Carbonic and high -carbon alloy steel often show unevenness. This unevenness is mainly manifested in carbide liquid analysis, carbide band -shaped, and carbide mesh.
1 Carbide liquid analysis
Carbonized liquid analysis is a sub -stabilized Gonglai Austenity produced by carbon and alloy elements in the liquid phase. During the heat processing, the carbide liquid analysis was broken into irregular pieces, and it was distributed in a chain or strip in the direction of the pressure extension.

Carbonized liquid analysis is due to the comprehensive result of the steel fluid overheating, the high watering temperature, the cooling of the steel ingot is too slow, and the chromium reducing the maximum solid solution of carbon in the auscles. It is generally believed that the carbide liquid analysis belongs to the carbide of the triangular crystal, and its hardness is extremely high. Its existence will cause the bearing parts to produce quenching cracks during thermal treatment. During the use process The liquid analysis of carbides can cause fatigue cracks and reduce fatigue life.
2 carbide strap
The carbide band is the crystalline bias (bias analysis) formed by the steel liquid in the solidification process, causing the carbon high and low concentration of different analytical bands.
After the rolling extension, a large number of excess overcover secondary carbides are precipitated from high concentrations during the cooling process, thereby forming a carbon band tissue of black and white (high and low carbon).

The final solidification zone of the steel ingot or casting is rich in a large amount of alloy elements, namely sulfur, phosphorus and other impurities. It is the most gathering area for non -metal mixed materials and carbides. The total amount and distribution status of carbides during the cooling process depends mainly on the degree of primitive analysis. With the intensification of carbonized band -shaped bias, the sensitivity of the cracking of thermal treatment increases, the microscopic hardness difference between high and low carbon belt increases, and affects the fatigue life of contact. Band -shaped carbides can be evaluated based on GB/T 1299 "Alloy Tool Steel".
3 carbide mesh
The carbide mesh is an excess carbide distributed in the network -shaped distribution of the cyber -shaped distribution of the borders of the co -analyzed steel. It is related to the chemical composition and bias of the steel. The uneven band is also a factor that affects the service life of the part. The carbide mesh can be evaluated based on GB/T 1298 "Carbon Tool Steel".

The picture above shows the micro -tissue of the T12 steel completely annealing. The dark sheet layer in the figure is pearl light, and the white mesh around it is a secondary carburizing body.
In summary, the uneven carbides in high -carbon steel and high -carbon high -alloy steel are essentially the result of the macro and micro -analysis of the steel liquid during the cooling process. Among the three, carbide solution is the most harmful. Although carbide liquid analysis is completely different from non -metallic mixed with non -metallic mixed in nature, as far as its harmfulness is concerned, carbide liquid analysis can be combined into the scope of the test of miscellaneous objects. To eliminate carbide solution, in essence, it is necessary to reduce the level of branches in the steel in the steel, so that the most severe area in the steel cannot form a common crystal Lai Aurona.
4 Bearing steel mesh carbide formation and harm
The mesh carbide was formed in the Austrian body crystal world during the high -end rolling temperature and the slow and cold process. Once the mesh carbides are formed, especially when the carbide is completely surrounded by the crystal world and is wide, it will have bad consequences during subsequent processing and use. First of all, the severe carbide mesh in bearing steel cannot be completely eliminated in the future ballization annealing. In this way, it is easy to cause grinding cracks during the grinding process of bearing processing, also known as cracking; second, if carbides, if carbides The mesh is serious, not only the ballization annealing cannot be eliminated, but even in the future quenching organization. In this case, it is easy to cause quenching cracks. Even if there is no cracking during quenching, carbonized The mesh will also easily cause fatigue cracks.
When a carbide mesh tissue in the bearing steel will increase the brittleness of the steel and reduce the fatigue life of the bearing parts. Therefore, no serious carbide mesh tissue is allowed in the bearing steel tissue in the use state.
5 How to eliminate carbonized mesh
High -carbon chromium bearing steel has a high carbon content, and contains a certain amount of carbides for forming elements. During the solidification process, these elements are prone to bias, resulting in uneven distribution of carbides in steel.
The measures taken to eliminate carbide mesh during the production process are as follows:
1) When smelting high -carbon chromium bearing steel, the content of carbon and chromium is strictly controlled to meet the requirements.
2) During the coagulation process of the steel ingot, the branch -like bias in the steel should be reduced and the level of carbides should be reduced.
3) Control the low -rolling temperature with a lower rolling, and speed up the cooling speed after rolling to reduce the carbonic level of bearing steel.
With the continuous development of rolling technology, the method of cooling after rolling has gradually been widely used, that is, on the basis of reducing the final rolling temperature, wind -cooling, water spraying, or cooling the sink through the sink after rolling. Practice has proved that when the final rolling temperature is less than 850 ° C, the Austrian body crystal is small, and it is cooled after rolling, which prevents the precipitation of the mesh carbide on the Aorer crystal world. It is better to eliminate mesh carbides?